solution and composite the horn

This is where we discuss the craft of bow and arrow making.
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Sun Oct 25, 2015 3:19 pm

when the all horn soluttion well the super stronger foul smell fulling all room and outdoor from 30M like 150 year ago the WC ,yes , i can soluttion horn form acid\enzymolysis, i find the glue of horn , it often in the top of liquid; the sheep horn glue seemed in the bottom, i need got a feeler mechanism know what it is and buy it , make it is need 3m mask for avoid these smell
You do not have the required permissions to view the files attached to this post.
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Sun Oct 25, 2015 3:20 pm

pic of sheep horn
You do not have the required permissions to view the files attached to this post.
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Sun Oct 25, 2015 3:24 pm

pic, the black horn in last drying step
You do not have the required permissions to view the files attached to this post.
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Thu Jan 14, 2016 7:35 am

the sheep horn on bow test,
You do not have the required permissions to view the files attached to this post.
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Thu Jan 14, 2016 7:36 am

pic
You do not have the required permissions to view the files attached to this post.
mikekeswick
Posts: 404
Joined: Tue May 05, 2009 11:01 am
Location: Durham,Engalnd

Post by mikekeswick » Thu Jan 14, 2016 8:00 am

What are you trying to do!!??
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Thu Jan 14, 2016 8:49 am

this is form soluttion horn for composite the horn
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Thu Jan 14, 2016 8:53 am

http://atarn.net/phpBB2/files/img_1754_973.jpg

it is not soluttion well , when it pull soluttion it become super glue but very hard dry it
pcoutin
Posts: 150
Joined: Thu Dec 03, 2015 11:40 am
Location: California
Contact:

Post by pcoutin » Thu Jan 14, 2016 10:00 am

So... somehow trying to make horn or a material that behaves like horn artificially? In a liquid solution that then dries?
would like to see tests
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Thu Jan 14, 2016 2:13 pm

the juyuanhao bowyer tell me and show me he make horn like this , so many difficulty step by step, yes , it is ,and use fiberglass do it more good than this, it is no more layer and fibre like the raw horn,
mikekeswick
Posts: 404
Joined: Tue May 05, 2009 11:01 am
Location: Durham,Engalnd

Post by mikekeswick » Sat Jan 16, 2016 8:01 am

So you are trying to make a solution of keratin from horn scraps that can be dried into a form that would then be used in place of normal horn strips on a bow?
pcoutin
Posts: 150
Joined: Thu Dec 03, 2015 11:40 am
Location: California
Contact:

Post by pcoutin » Sat Jan 16, 2016 8:29 am

and use fiberglass do it more good than this, it is no more layer and fibre like the raw horn,
so you think fiberglass would end up being better? "dried horn" wouldn't be able to bend as much as real horn?
User avatar
jiao
Posts: 663
Joined: Fri May 06, 2005 1:24 pm
Location: china
Contact:

Post by jiao » Sun Jan 17, 2016 6:52 am

now the big trouble is dry and apply the horn "glue", the horn glue on hand or touch anything, very hard remove it , so easy hang a edge of a knife on a steel dish

lot test need i do it , i am not genius plese waiting
Post Reply